Additional services: To ensure our customers' processes and/or products attain – and even exceed – their performance expectations, we offer a wide range of services within both the technical area and delivery logistics. Our technical services include: • Material consultations through our worldwide sales network • Advice in process optimization based on an in-depth applications knowledge • Joint new product development supported by our extensive R&D program View product groups and servicesProperties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.94 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 201 GPa | |
20.0 °C | 194 GPa | ||
100.0 °C | 189 GPa | ||
200.0 °C | 183 GPa | ||
300.0 °C | 177 GPa | ||
400.0 °C | 170 GPa | ||
500.0 °C | 163 GPa | ||
600.0 °C | 156 GPa | ||
700.0 °C | 149 GPa | ||
800.0 °C | 141 GPa | ||
900.0 °C | 134 GPa | ||
1000.0 °C | 127 GPa | ||
Elongation | 20.0 °C | 35 % | |
Elongation, transverse | 20.0 °C | 30 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] | Typical for Austenitic Stainless Steel |
Shear modulus | 23.0 °C | 77 GPa | Typical for Austenitic Stainless Steel |
Tensile strength | 20.0 °C | 500 - 750 MPa | |
Tensile strength, transverse | 20.0 °C | 500 - 750 MPa | |
Yield strength Rp0.2 | 20.0 °C | 210 MPa | |
100.0 °C | 180 MPa | ||
200.0 °C | 160 MPa | ||
300.0 °C | 145 MPa | ||
400.0 °C | 130 MPa | ||
500.0 °C | 120 MPa | ||
550.0 °C | 115 MPa | ||
600.0 °C | 110 MPa | ||
Yield strength Rp0.2, transverse | 20.0 °C | 210 MPa | |
Yield strength Rp1.0 | 20.0 °C | 240 MPa | |
100.0 °C | 205 MPa | ||
200.0 °C | 180 MPa | ||
300.0 °C | 165 MPa | ||
400.0 °C | 155 MPa | ||
500.0 °C | 145 MPa | ||
550.0 °C | 140 MPa | ||
600.0 °C | 135 MPa | ||
Yield strength Rp1.0, transverse | 20.0 °C | 240 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.36E-5 1/K | |
20.0 °C | 1.46E-5 1/K | ||
100.0 °C | 1.51E-5 1/K | ||
200.0 °C | 1.57E-5 1/K | ||
300.0 °C | 1.62E-5 1/K | ||
400.0 °C | 1.66E-5 1/K | ||
500.0 °C | 1.7E-5 1/K | ||
600.0 °C | 1.74E-5 1/K | ||
700.0 °C | 1.77E-5 1/K | ||
800.0 °C | 1.8E-5 1/K | ||
900.0 °C | 1.83E-5 1/K | ||
1000.0 °C | 1.86E-5 1/K | ||
Melting point | 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) | |
20.0 °C | 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 11.5 W/(m·K) | |
100.0 °C | 13.1 W/(m·K) | ||
200.0 °C | 14.8 W/(m·K) | ||
300.0 °C | 16.4 W/(m·K) | ||
400.0 °C | 18.1 W/(m·K) | ||
500.0 °C | 19.6 W/(m·K) | ||
600.0 °C | 21.2 W/(m·K) | ||
700.0 °C | 22.8 W/(m·K) | ||
800.0 °C | 24.3 W/(m·K) | ||
900.0 °C | 25.7 W/(m·K) | ||
1000.0 °C | 27.3 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 3.1 mm²/s | |
100.0 °C | 3.3 mm²/s | ||
200.0 °C | 3.6 mm²/s | ||
300.0 °C | 3.9 mm²/s | ||
400.0 °C | 4.2 mm²/s | ||
500.0 °C | 4.4 mm²/s | ||
600.0 °C | 4.6 mm²/s | ||
700.0 °C | 4.9 mm²/s | ||
800.0 °C | 5.2 mm²/s | ||
900.0 °C | 5.5 mm²/s | ||
1000.0 °C | 5.7 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 1.01E-6 Ω·m |
100.0 °C | 1.04E-6 Ω·m | |
200.0 °C | 1.08E-6 Ω·m | |
300.0 °C | 1.12E-6 Ω·m | |
400.0 °C | 1.15E-6 Ω·m | |
500.0 °C | 1.18E-6 Ω·m | |
600.0 °C | 1.2E-6 Ω·m | |
700.0 °C | 1.22E-6 Ω·m | |
800.0 °C | 1.24E-6 Ω·m | |
900.0 °C | 1.26E-6 Ω·m | |
1000.0 °C | 1.27E-6 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Aluminium | 0.2 - 0.5 % |
Carbon | 0.03 - 0.08 % |
Chromium | 19 - 22 % |
Cobalt | 0.5 % |
Copper | 0.5 % |
Manganese | 1.5 % |
Nickel | 30 - 32.5 % |
Niobium | 0.1 % |
Phosphorus | 0.02 % |
Silicon | 0.7 % |
Sulfur | 0.01 % |
Titanium | 0.2 - 0.5 % |
Metal
- EN 10222-5 X2CrNiMo18-14-3 Solution‑Annealed Grade for Corrosion‑Resistant Applications
- EN 1652 Grade CuSn4 – Recrystallized & Annealed for Optimal Formability & Strength
- EN 10222-5 X6CrNiMoTi17-12-2 (Solution Annealed) – High Corrosion‑Resistant Stainless Steel
- EN 10222-5 X6CrNiTi18-10 – Solution Annealed & AT: Premium Corrosion‑Resistant Steel for Chemical & Food Applications
- X2CrNiMo18-14-3 Solution Annealed – EN 10250-4 Grade, Superior Corrosion Resistance
- EN 10216‑5 X6CrNiMoTi17‑12‑2: Solution‑Annealed Stainless Steel with Enhanced Corrosion Resistance
- EN 10216-5 X2CrNiMo18-14-3 Solution-Annealed Steel (+AT) – Superior Corrosion Resistance
- EN 10216-5 Grade X5CrNi18-10 Solution Annealed (+AT) – High Corrosion Resistance Stainless Steel
- EN 10216-5 X6CrNiTi18-10 Solution-Annealed – Titanium‑Stabilized Stainless Steel with Superior Corrosion Resistance & Weldability
- EN 10028‑7 X5NiCrAlTi31‑20 +RA: Heat‑Resistant Austenitic Steel for Pressure Vessels