DIN 1725-1 (Grade 3.3523 G25) – Superior Corrosion-Resistant Aluminum Alloy
Aluminum DIN 3.3523 is a non-heat treatable alloy with excellent finishing qualities. DIN 3.3523 offers better corrosion resistance than most aluminum alloys, especially to salt water and marine atmospheres. This alloy can be readily welded using most common techniques and is in fact offers some of the best welding characteristics of all aluminum alloys.
Properties
General
| Property | Temperature | Value | Condition | Related Standards |
|---|---|---|---|---|
Density | 20.0 °C | 2.68 g/cm³ | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Mechanical
| Property | Temperature | Value | Condition | Related Standards | Comment |
|---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 72.0 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
Elongation | -196.0 °C | 28.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
-80.0 °C | 21.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
-28.0 °C | 18.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
20.0 °C | 16.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
100.0 °C | 18.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
150.0 °C | 27.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
200.0 °C | 45.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
260.0 °C | 80.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
315.0 °C | 110.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
370.0 °C | 130.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | |||
Poisson's ratio | 0.33 [-] | Typical for Wrought 5000 Series Aluminium | |||
Shear modulus | 20.0 °C | 27.0 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
Tensile strength | -196.0 °C | 380.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
-80.0 °C | 280.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
-28.0 °C | 260.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
20.0 °C | 260.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
100.0 °C | 260.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
150.0 °C | 205.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
200.0 °C | 165.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
260.0 °C | 85.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
315.0 °C | 50.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
370.0 °C | 35.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Thermal
| Property | Temperature | Value | Condition | Related Standards | Comment |
|---|---|---|---|---|---|
Coefficient of thermal expansion | -50.0 °C | 2.21e-05 1/K | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
100.0 °C | 2.38e-05 1/K | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
200.0 °C | 2.48e-05 1/K | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
300.0 °C | 2.57e-05 1/K | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
Max service temperature | 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Melting point | 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Specific heat capacity | 20.0 °C | 900.0 J/(kg·K) | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
Thermal conductivity | 20.0 °C | 150.0 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Electrical
| Property | Temperature | Value | Condition | Related Standards | Comment |
|---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 21000000.0 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
Electrical resistivity | 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
| Property | Value | Condition | Related Standards |
|---|---|---|---|
Chromium | 0.15 - 0.35 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Copper | 0.1 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Iron | 0.4 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Magnesium | 2.2 - 2.8 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Manganese | 0.1 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Silicon | 0.25 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Zinc | 0.1 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Technological properties
| Property | ||
|---|---|---|
| Workability | Good workability. | |
Metal
- DIN 1725-1 Grade 3.4415 – High-Performance Al–Zn Alloy for Corrosion Protection
- DIN 1725-1 Grade 3.2315 T5 Aluminum Tube – Technical Specifications
- DIN 1725-1 Grade 3.3523 (H34) – High‑Performance, Corrosion‑Resistant Aluminum Alloy
- DIN 1725-1 Grade 3.4365 T5 – High‑Strength 7075 Aluminum Alloy for Aerospace
- DIN 1725‑1 Grade 3.4365 O – Premium High‑Strength Aluminum Alloy for Aerospace
- DIN 1725-1 Grade 3.4335 T5 Aluminum Alloy – High-Performance Wrought Grade
- DIN 1725-1 Grade 3.3211 T8 Alloy: Superior Corrosion Resistance & Finish
- DIN 1725-1 Grade 3.0615 T8: High-Performance Free-Cutting Alloy
- DIN 1725-1 Grade 3.1255 T8 Aluminum Alloy – High Strength & Precision Machining
- DIN 1725-1 Grade 3.3523 T6 – High-Performance Aluminum Alloy