The make X4CrNiMo16-5-1 is comparable to X 4 CrNiMo 16 5 acc. to SEW400 : 1991-02. The material is a martensitic stainless steel for machine engineering, for pumps, instruments, compressor and in shipbuilding. It shows favorable corrosion resistance and low temperature ductility up to -200°C. Furthermore it shows high corrosion resistance particularly to water, weak acids and bases, oxidizing acids (nitrous acid) and weakly chloride-containing media.
Quantity: 300 EURAdditional services: Project based stainless steel packages for long, flat and tubular products. Implementing specs, approving mills and productions outfits, planning production finished and pre material routes. Making sure delivery is on time. Forgings, centrifugal casting, HIP products. Sourcing of materialUGITECH
MANUFACTURER
Information and services
Additional services: https://eservices.ugitech.com/Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.56 - 7.7 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | 20.0 °C | 200 - 218 GPa | |
100.0 °C | 195 - 213 GPa | ||
200.0 °C | 185 - 206 GPa | ||
300.0 °C | 175 - 198 GPa | ||
400.0 °C | 190 GPa | ||
500.0 °C | 180 GPa | ||
600.0 °C | 167 GPa | ||
700.0 °C | 150 GPa | ||
Elongation | 20.0 °C | 16 % | |
Elongation, transverse | 20.0 °C | 14 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] | Typical for Martensitic Stainless Steel |
Shear modulus | 23.0 °C | 77 GPa | Typical for Martensitic Stainless Steel |
Tensile strength | 20.0 °C | 760 - 1100 MPa | |
Tensile strength, transverse | 20.0 °C | 760 - 1100 MPa | |
Yield strength Rp0.2 | 20.0 °C | 550 - 750 MPa | |
100.0 °C | 520 - 660 MPa | ||
150.0 °C | 510 - 640 MPa | ||
200.0 °C | 500 - 620 MPa | ||
250.0 °C | 490 - 600 MPa | ||
300.0 °C | 480 - 580 MPa | ||
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | 20.0 °C | 9.9E-6 1/K | |
100.0 °C | 1.03E-5 1/K | ||
200.0 °C | 1.08E-5 1/K | ||
300.0 °C | 1.12E-5 1/K | ||
400.0 °C | 1.16E-5 1/K | ||
500.0 °C | 1.19E-5 1/K | ||
600.0 °C | 1.21E-5 1/K | ||
700.0 °C | 1.24E-5 1/K | ||
800.0 °C | 1.29E-5 1/K | ||
Melting point | 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Specific heat capacity | 20.0 °C | 430 - 450 J/(kg·K) | |
100.0 °C | 482 J/(kg·K) | ||
200.0 °C | 506 J/(kg·K) | ||
300.0 °C | 525 J/(kg·K) | ||
400.0 °C | 547 J/(kg·K) | ||
500.0 °C | 576 J/(kg·K) | ||
600.0 °C | 616 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 15 - 16 W/(m·K) | |
100.0 °C | 17.2 W/(m·K) | ||
200.0 °C | 18.6 W/(m·K) | ||
300.0 °C | 20 W/(m·K) | ||
400.0 °C | 21.2 W/(m·K) | ||
500.0 °C | 22.3 W/(m·K) | ||
600.0 °C | 23.3 W/(m·K) | ||
700.0 °C | 24.1 W/(m·K) | ||
800.0 °C | 25.5 W/(m·K) | ||
900.0 °C | 26.9 W/(m·K) | ||
1000.0 °C | 28.3 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 4.7 mm²/s | |
100.0 °C | 4.5 mm²/s | ||
200.0 °C | 4.5 mm²/s | ||
300.0 °C | 4.6 mm²/s | ||
400.0 °C | 4.4 mm²/s | ||
500.0 °C | 4.1 mm²/s | ||
600.0 °C | 3.6 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 9.06E-7 Ω·m |
100.0 °C | 9.42E-7 Ω·m | |
200.0 °C | 9.87E-7 Ω·m | |
300.0 °C | 1.03E-6 Ω·m | |
400.0 °C | 1.08E-6 Ω·m | |
500.0 °C | 1.12E-6 Ω·m | |
600.0 °C | 1.18E-6 Ω·m | |
700.0 °C | 1.22E-6 Ω·m | |
800.0 °C | 1.24E-6 Ω·m | |
900.0 °C | 1.26E-6 Ω·m | |
1000.0 °C | 1.27E-6 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.06 % |
Chromium | 15 - 17 % |
Manganese | 1.5 % |
Molybdenum | 0.8 - 1.5 % |
Nickel | 4 - 6 % |
Nitrogen | 0.02 % |
Phosphorus | 0.04 % |
Silicon | 0.7 % |
Sulfur | 0.03 % |
Metal
- EN 10250‑4 Grade X12Cr13 – Quenched & Tempered Stainless Steel for Industrial Applications
- EN 10250-4 Grade X20Cr13 Quenched & Tempered Steel – High Strength, Corrosion Resistant
- EN 10250-4 X30Cr13 Quenched & Tempered Steel – Ideal for Cutting Tools & High‑Wear Parts
- EN 10213 Grade GX23CrMoV12-1: Quenched and Tempered Steel for High‑Temperature Applications
- EN 10028-7 Grade X4CrNiMo16-5-1: High-Performance Quenched & Tempered Martensitic Stainless Steel
- EN 10250-4 Grade X17CrNi16-2 – Quenched & Tempered Steel for High-Load Applications
- EN 10250-4 Grade X3CrNiMo13-4: High-Performance Quenched & Tempered Steel for Turbines & Power Plants
- X4CrNiMo16-5-1 Grade: Quenched & Tempered (QT900) – High‑Performance Martensitic Stainless Steel
- EN 10272 Grade X4CrNiMo16-5-1 (QT900) – Premium Quenched & Tempered Steel for Pressure Vessels
- EN 10272 Grade X4CrNiMo16-5-1 Quenched & Tempered Steel (+QT760) – High-Performance Corrosion Resistance